您好,歡迎訪問禹城泰瑞彩鋼復合板加工廠!

服務熱線

18765446878

熱門關鍵詞:禹城彩鋼廠,禹城彩鋼復合板,禹城鋼結構板房 彩鋼板房

彩鋼使用中會出現的質量問題

來源:http://www.cygpw.cn 日期:2022-07-25 發布人:
彩鋼板是指彩涂鋼板,是一種帶有有機涂層的鋼板,可以說是人們較為熟悉的板材,當然使用時候會發生的質量問題是不可避免的,下面濟南彩鋼小編來列舉幾項,提前了解并預防。
Color steel plate refers to color coated steel plate, which is a kind of steel plate with organic coating. It can be said that it is a familiar plate. Of course, the quality problems that will occur when used are inevitable. The following Jinan color steel editor will list several items to understand and prevent in advance.
彎曲性不良(T彎)
Poor bending (T-bend)
鋼材彎曲180度試驗時,加工部位的涂層發生龜裂及涂層剝離。
During the 180 degree bending test of steel, the coating on the processing part cracks and peels off.
發生原因: 1、前處理的掌握量過多。2、涂層厚度過厚。3、過度烘烤。4、下涂涂料同上涂涂料的制造廠家不同,或稀料的使用不當。
Causes: 1. Too much pre-treatment. 2. The coating thickness is too thick. 3. Over bake. 4. The lower coating is different from the manufacturer of the coating, or the thinner is improperly used.
邊部氣泡
Edge bubble
兩側沾有涂料,經烘干,出現氣泡。
There is paint on both sides. After drying, bubbles appear.
發生原因:原材有毛刺沾有涂料多,兩邊出現縫隙。
Cause of occurrence: raw materials have burrs and paint, and cracks appear on both sides.
麻點
Pitting
特點:從外部混入的異物或灰塵在涂裝后,部分或全部表面,有米粒樣的突出。
Features: foreign matters or dust mixed from the outside will protrude on some or all surfaces after coating.
發生原因:1、涂料中混入其它種類或其它公司的涂料。2、涂料中有異物混入引起。3、前處理過程中水洗不良。
Causes: 1. The paint is mixed with other kinds of paint or paint from other companies. 2. It is caused by the mixing of foreign matters in the paint. 3. Poor washing during pretreatment.
橘皮
Orange peel
特點:已干燥的表面涂層象橘子皮一樣粗糙,不均勻。
Features: the dried surface coating is as rough and uneven as orange peel.
發生原因:1、濕膜過厚。2、涂料的黏度較高時。
Causes: 1. The wet film is too thick. 2. When the viscosity of paint is high.
耐溶劑性能差(MEK)
Poor solvent resistance (MEK)
特點:擦拭有點狀掉漆。
Features: there are dots of paint falling off after wiping.
發生原因:1、烘烤溫度沒有達到要求。 2、涂料的固化有問題。3、前處理清洗不干凈。
Causes: 1. The baking temperature did not meet the requirements. 2. There is a problem with the curing of the coating. 3. The pretreatment and cleaning are not clean.
濟南彩鋼
縮孔
Shrinkage cavity
特點: 漆膜不平整,局部露底。
Features: the paint film is uneven and partially exposed.
發生原因:1、鋼帶表面不潔凈。2、底漆冷卻水不潔凈。3、涂料粘度沒達到上機要求。
Causes: 1. The steel strip surface is not clean. 2. The cooling water of primer is not clean. 3. The viscosity of the coating did not meet the requirements of the machine.
漏涂
Holiday coating
特點:面漆未涂上。
Features: topcoat is not applied.
發生原因:1、邊部面漆未涂上,基板板型不好或涂輥與大背輥間壓力不足。2、板面中間面漆未涂上,底漆冷卻后板面有水或其它異物。
Causes: 1. The edge finish paint is not applied, the base plate shape is not good, or the pressure between the coating roll and the large back roll is insufficient. 2. The middle finish of the plate surface is not painted, and there is water or other foreign matters on the plate surface after the primer is cooled.
塌卷
Collapse roll
特點:鋼卷卷取后在倉庫存儲時內徑變形。
Features: the inner diameter of the steel coil is deformed when it is stored in the warehouse after coiling.
發生原因: 1、鋼卷卷取后受外力的影響。2、收卷張力不正確。3、荷重不均。
Causes: 1. The steel coil is affected by external force after coiling. 2. The winding tension is incorrect. 3. Uneven load.
反粘
Anti adhesion
特點:開卷時有輕度剝離,底漆返沾會出現類似小米粒狀顆粒,涂面漆后表面凹凸不平。
Features: there is slight peeling when uncoiling, and there will be particles similar to millet particles when the primer is back stained, and the surface will be uneven after coating the top coat.
發生原因:1、卷取前冷卻不夠。2、烘烤不足。3、部分載重過大。
Causes: 1. Insufficient cooling before coiling. 2. Insufficient baking. 3. Part of the load is too large.
壓傷
Crush injury
特點:在涂敷之后的壓坑。
Features: pressure pit after coating.
發生原因:1、原料卷有壓傷。2、在涂敷之前通過各種輥子壓傷。3、在涂敷之后和涂料一塊的壓傷。
Causes: 1. The raw material roll is crushed. 2. Crush by various rollers before coating. 3. Crushing with paint after coating.
彩鋼使用中會出現的質量問題就是如上了,如果您對其還存有疑惑的話,歡迎來此網站http://www.cygpw.cn進行咨詢!
The quality problems in the use of color steel are as above. If you still have doubts about it, welcome to this website http://www.cygpw.cn Consult!

聯系電話:18765446878

咨詢熱線:18765446878(微信同號)

地址:禹城市十里望鎮山東國際商貿港往南660米

備案號:魯ICP備2023024436號 魯公網安備37010202001695號 網站地圖|XML|TXT

微信二維碼

微信二維碼

主站蜘蛛池模板: 中红外QCL激光器-其他连续-半导体连续激光器-筱晓光子 | 深圳标识制作公司-标识标牌厂家-深圳广告标识制作-玟璟广告-深圳市玟璟广告有限公司 | 除甲醛公司-甲醛检测-广西雅居环境科技有限公司 | 活性炭-蜂窝-椰壳-柱状-粉状活性炭-河南唐达净水材料有限公司 | 空调风机,低噪声离心式通风机,不锈钢防爆风机,前倾皮带传动风机,后倾空调风机-山东捷风风机有限公司 | 贴片电容-贴片电阻-二三极管-国巨|三星|风华贴片电容代理商-深圳伟哲电子 | 希望影视-高清影视vip热播电影电视剧免费在线抢先看 | 深圳侦探联系方式_深圳小三调查取证公司_深圳小三分离机构 | 成都亚克力制品,PVC板,双色板雕刻加工,亚克力门牌,亚克力标牌,水晶字雕刻制作-零贰捌广告 | 磁棒电感生产厂家-电感器厂家-电感定制-贴片功率电感供应商-棒形电感生产厂家-苏州谷景电子有限公司 | 薄壁轴承-等截面薄壁轴承生产厂家-洛阳薄壁精密轴承有限公司 | 新密高铝耐火砖,轻质保温砖价格,浇注料厂家直销-郑州荣盛窑炉耐火材料有限公司 | 广州工业氧气-工业氩气-工业氮气-二氧化碳-广州市番禺区得力气体经营部 | 期货软件-专业期货分析软件下载-云智赢 | 粤丰硕水性环氧地坪漆-防静电自流平厂家-环保地坪涂料代理 | 卧涛科技有限公司科技项目申报公司|高新技术企业申报|专利申请 | 陶瓷砂磨机,盘式砂磨机,棒销式砂磨机-无锡市少宏粉体科技有限公司 | 影视模板素材_原创专业影视实拍视频素材-8k像素素材网 | 储能预警-储能消防系统-电池舱自动灭火装置-四川千页科技股份有限公司官网 | 立式_复合式_壁挂式智能化电伴热洗眼器-上海达傲洗眼器生产厂家 理化生实验室设备,吊装实验室设备,顶装实验室设备,实验室成套设备厂家,校园功能室设备,智慧书法教室方案 - 东莞市惠森教学设备有限公司 | 探伤仪,漆膜厚度测试仪,轮胎花纹深度尺厂家-淄博创宇电子 | 北京网站建设首页,做网站选【优站网】,专注北京网站建设,北京网站推广,天津网站建设,天津网站推广,小程序,手机APP的开发。 | 超声波成孔成槽质量检测仪-压浆机-桥梁预应力智能张拉设备-上海硕冠检测设备有限公司 | 除尘器布袋骨架,除尘器滤袋,除尘器骨架,电磁脉冲阀膜片,卸灰阀,螺旋输送机-泊头市天润环保机械设备有限公司 | 清洁设备_洗地机/扫地机厂家_全自动洗地机_橙犀清洁设备官网 | 临海涌泉蜜桔官网|涌泉蜜桔微商批发代理|涌泉蜜桔供应链|涌泉蜜桔一件代发 | 橡胶膜片,夹布膜片,橡胶隔膜密封,泵阀设备密封膜片-衡水汉丰橡塑科技公司网站 | 新能源汽车电机定转子合装机 - 电机维修设备 - 睿望达 | 济南品牌包装设计公司_济南VI标志设计公司_山东锐尚文化传播 | 四探针电阻率测试仪-振实密度仪-粉末流动性测定仪-宁波瑞柯微智能 | 代理记账_免费注册公司_营业执照代办_资质代办-【乐财汇】 | 莱州网络公司|莱州网站建设|莱州网站优化|莱州阿里巴巴-莱州唯佳网络科技有限公司 | 称重传感器,测力传感器,拉压力传感器,压力变送器,扭矩传感器,南京凯基特电气有限公司 | 耐磨陶瓷管道_除渣器厂家-淄博浩瀚陶瓷科技有限公司 | 公交驾校-北京公交驾校欢迎您!| 台式核磁共振仪,玻璃软化点测定仪,旋转高温粘度计,测温锥和测温块-上海麟文仪器 | 重庆小面培训_重庆小面技术培训学习班哪家好【终身免费复学】 | 道达尔润滑油-食品级润滑油-道达尔导热油-合成导热油,深圳道达尔代理商合-深圳浩方正大官网 | 可程式恒温恒湿试验箱|恒温恒湿箱|恒温恒湿试验箱|恒温恒湿老化试验箱|高低温试验箱价格报价-广东德瑞检测设备有限公司 | 防水套管_柔性防水套管_刚性防水套管-巩义市润达管道设备制造有限公司 | 稳尚教育加盟-打造高考志愿填报平台_新高考志愿填报加盟_学业生涯规划加盟 |